產(chǎn)品詳情
OK 67.50瑞典伊薩焊材 E2209-17不銹鋼焊條
是一款適用于焊接CrNiMoN 22 5 3 和CrNiN 23 4牌號奧氏體-鐵素體不銹鋼的酸性金紅石藥皮焊條。其雙相全焊縫金屬具有高強度與優(yōu)良延展性相結(jié)合的特點。 抗點蝕性能優(yōu)良,且全焊縫金屬不易受到應(yīng)力腐蝕開裂的影響。
Typical Tensile Properties
As welded
Elongation
Tensile Strength
Yield Strength
保護氣體
25 %
857 MPa
691 MPa
ISO
-
-
-
AWS
夏比V型缺口沖擊性能
As welded
Impact Value
Testing Temperature
保護氣體
50 J
20 °C
ISO
41 J
-30 °C
ISO
焊縫金屬分析
Mn
Mn
Mo
C
Si
Ferrite FN
Ni
N
Cr
0.8 %
-
-
-
-
-
-
-
Mo
Mn
Mo
C
Si
Ferrite FN
Ni
N
Cr
-
3.2 %
-
-
-
-
-
-
C
Mn
Mo
C
Si
Ferrite FN
Ni
N
Cr
-
-
0.03 %
-
-
-
-
-
Si
Mn
Mo
C
Si
Ferrite FN
Ni
N
Cr
-
-
-
0.8 %
-
-
-
-
Ferrite FN
Mn
Mo
C
Si
Ferrite FN
Ni
N
Cr
-
-
-
-
42 %
-
-
-
Ni
Mn
Mo
C
Si
Ferrite FN
Ni
N
Cr
-
-
-
-
-
8.8 %
-
-
Cr
Mn
Mo
C
Si
Ferrite FN
Ni
N
Cr
-
-
-
-
-
-
-
23.2 %
熔敷數(shù)據(jù)
Fusion time per electrode at 90% I max
kg weld bl/kg electrodes
Number of electrodes/kg weld bl
安培
熔敷率
電壓 V
直徑
33 sec
0.55 kg
152
30-65 A
0.7 kg/h
29 V
2.0 x 300 mm
38 sec
0.58 kg
91
50-90 A
1.0 kg/h
27 V
2.5 x 300 mm
55 sec
0.58 kg
47
80-120 A
1.4 kg/h
28 V
3.2 x 350 mm
59 sec
0.58 kg
32
90-160 A
1.9 kg/h
29 V
4.0 x 350 mm
64 sec
0.58 kg
20
150-220 A
2.8 kg/h
30 V
5.0 x 350 mm
OK 67.50瑞典伊薩焊材 E2209-17不銹鋼焊條
是一款適用于焊接CrNiMoN 22 5 3 和CrNiN 23 4牌號奧氏體-鐵素體不銹鋼的酸性金紅石藥皮焊條。其雙相全焊縫金屬具有高強度與優(yōu)良延展性相結(jié)合的特點。 抗點蝕性能優(yōu)良,且全焊縫金屬不易受到應(yīng)力腐蝕開裂的影響。
Typical Tensile Properties
As welded | |||
Elongation | Tensile Strength | Yield Strength | 保護氣體 |
25 % | 857 MPa | 691 MPa | ISO |
- | - | - | AWS |
夏比V型缺口沖擊性能
As welded | ||
Impact Value | Testing Temperature | 保護氣體 |
50 J | 20 °C | ISO |
41 J | -30 °C | ISO |
焊縫金屬分析
Mn | |||||||
Mn | Mo | C | Si | Ferrite FN | Ni | N | Cr |
0.8 % | - | - | - | - | - | - | - |
Mo | |||||||
Mn | Mo | C | Si | Ferrite FN | Ni | N | Cr |
- | 3.2 % | - | - | - | - | - | - |
C | |||||||
Mn | Mo | C | Si | Ferrite FN | Ni | N | Cr |
- | - | 0.03 % | - | - | - | - | - |
Si | |||||||
Mn | Mo | C | Si | Ferrite FN | Ni | N | Cr |
- | - | - | 0.8 % | - | - | - | - |
Ferrite FN | |||||||
Mn | Mo | C | Si | Ferrite FN | Ni | N | Cr |
- | - | - | - | 42 % | - | - | - |
Ni | |||||||
Mn | Mo | C | Si | Ferrite FN | Ni | N | Cr |
- | - | - | - | - | 8.8 % | - | - |
Cr | |||||||
Mn | Mo | C | Si | Ferrite FN | Ni | N | Cr |
- | - | - | - | - | - | - | 23.2 % |
熔敷數(shù)據(jù)
Fusion time per electrode at 90% I max | kg weld bl/kg electrodes | Number of electrodes/kg weld bl | 安培 | 熔敷率 | 電壓 V | 直徑 |
33 sec | 0.55 kg | 152 | 30-65 A | 0.7 kg/h | 29 V | 2.0 x 300 mm |
38 sec | 0.58 kg | 91 | 50-90 A | 1.0 kg/h | 27 V | 2.5 x 300 mm |
55 sec | 0.58 kg | 47 | 80-120 A | 1.4 kg/h | 28 V | 3.2 x 350 mm |
59 sec | 0.58 kg | 32 | 90-160 A | 1.9 kg/h | 29 V | 4.0 x 350 mm |
64 sec | 0.58 kg | 20 | 150-220 A | 2.8 kg/h | 30 V | 5.0 x 350 mm |